GH4145 alloy is a kind of corrosion-resistant, oxidation-resistant and high-strength precipitation hardening alloy. It is mainly a nickel-based superalloy that is aged and strengthened by γ"[Ni3(Al, Ti, Nb)] phase. It has good resistance below 980°C. Corrosion and oxidation resistance, high strength below 800℃, good relaxation resistance below 540℃, good formability and welding performance, and excellent mechanical properties in low temperature environments. The alloy is It has good corrosion resistance and creep rupture strength under high temperature environment, good mechanical properties, and is widely used: 1. Manufacturing springs and bolts that work at high temperatures; rotor blades, impellers and other structural parts on gas turbines; 2. The thrust chamber on the rocket engine; 3. Thrust reverse device on the aircraft; 4. Large high-pressure vessel; 5. Elastic air sealing sheet, elastic sealing die sheet, rubber mechanical electric heating blade. Chengyuan Alloy can supply various specifications of bars, forgings, ring parts, hot-rolled plates, cold-rolled plates, strips, pipes and wires of GH4145 grades. Plates and strips are generally supplied after hot rolling or cold rolling, annealing or solid solution, pickling and polishing. Bars, forgings and ring parts can be supplied in the forged or hot rolled state; they can also be supplied after forging and solution treatment; the bars can be supplied after solid solution and polished or turned. GH4145 chemical composition%
C
Cr
Ni+Co
Al
Cu
Fe
Ti
≤0.08
14.0~17.0
≥70
0.40~1.0
0.5
5.0~9.0
2.25~2.75
Nb+Ta
Co
S
Mn
Si
P
Mg
0.7~1.2
≤1.00
≤0.01
≤1.0
≤0.5
≤0.015
-
GH4145 thermal conductivity
θ/℃
50
100
300
500
900
λ/(W/(m•C))
14.7
15.9
20.1
25.1
37.3
GH4145 coefficient of linear expansion
θ/℃
20~200
20~300
20~400
20~500
20~600
20~700
20~800
α/10-6C-1
13.1
13.5
14.1
14.4
15.0
15.6
16.2
GH4145 physical properties
density
Melting point
Magnetic properties
g/cm3
℃
8.25
1395-1425
Non
Mechanical properties of GH4145 alloy at room temperature
Heat treatment method
Yield Strength
tensile strength
Elongation
Brinell hardness
Mpa,≥
Mpa,≥
%,≥
HB
Solution treatment
790
1170
10
302~363
Supply form and specification
Alloy grade
Form
Specification
GH4145
Wire
Diameter=0.03mm~8mm
GH4145
Flat wire
Width=0.4~40mm
Thick=0.03~2.9mm
GH4145
Strip
width=8~250mm
ThickT=0.1~3.0mm
GH4145
Foil
width=6~120mm
Thick=0.003~0.1mm
GH4145
Bar
Diameter=8~100mm
Long=50~1000
Superalloy Series: GH3030 GH4145 GH4169 Hastelloy C2 Hastelloy C4 Hastelloy C276 Hastelloy X Incoloy 800H Incoloy 825 Inconel 600 Inconel 625 Inconel 718 Inconel 725 Inconel X750 Monel 400 Monel K500 Nimonic 75A Nimonic263 Shijiazhuang Chengyuan Alloy Material Co., Ltd. is a high-tech enterprise specializing in the production of various alloy materials. It has an advanced and complete production line, including material smelting, surface cleaning, rolling, slitting, and a complete test process. Meet the corresponding quality inspection of different products. The company focuses on the production and supply of various electric heating alloys, expansion alloys, soft magnetic alloys, elastic alloys, high temperature alloys and all kinds of pure metals. The product forms include wire, flat wire, strip, plate, bar, foil, Seamless pipe, wire mesh, powder, etc. can meet the application needs of different customers. The various performance indicators of the product are strictly in accordance with the national standards. If customers put forward non-standard requirements, they can also be implemented by reference.Our products are widely used in heating equipment, machinery manufacturing, electric furnace production, instrumentation, household appliances, mineral mining, aerospace, petroleum and nuclear power and other industries, and have received good market feedback. Our products have stable delivery time, excellent quality, sophisticated packaging, and high repurchase rate. They are not only widely recognized in the domestic market, but also have a good reputation in the international market.* OEM manufacturer* We will deliver the goods to the warehouse of the customer's agent in any city in China.* Terms of delivery: EXW, FCA, FOB, CIF, CPT, DAP* Mode of transport: Sea, Auto, Railway, Air and Express* Payment terms: Bank Transfer, Western Union, PayPal, Alipay* Quality Certificate:In order to improve the quality of products and services, with each order we provide a quality certificate for goods, which includes measured data - chemical composition, electrical resistivity, tensile strength, elongation, melting number, etc.Cheng Yuan Alloy Material Co., LtdEmail: [email protected]Tel .: +86 13673186216+86 311 8803 3197